Akulon® S223-G6-FC NA99001

30% Glass Fiber Reinforced, Food Contact Quality

General Information

Akulon® is our family of high performance polyamide 6 and polyamide 66 materials, used by customers across the world in applications ranging from automotive, electronics & electrical, to furniture and packaging.
We offer Akulon® grades for injection molding, blow molding and extrusion (including barrier film, stock shapes, convoluted tubes, and mono and multi filament).
In molded parts the material offers an excellent balance of easy design and processing with outstanding mechanical properties over a wide temperature range and in diverse conditions. Meanwhile for extrusion the strength, resilience and easy processing of Akulon® sets the market standards.
Special features
Regulatory Affairs
Processing technology
Injection Molding

Rheological properties

Molding shrinkage [parallel]
0.2
%
Molding shrinkage [normal]
1.2
%

Mechanical properties

Tensile modulus
10000
MPa
Tensile modulus (-40°C)
10500
MPa
Tensile modulus (100°C)
4850
MPa
Tensile modulus (120°C)
4550
MPa
Tensile modulus (150°C)
4100
MPa
Tensile modulus (160°C)
3950
MPa
Tensile modulus (180°C)
3650
MPa
Tensile modulus (200°C)
3350
MPa
Stress at break
200
MPa
Stress at break (-40°C)
250
MPa
Stress at break (100°C)
110
MPa
Stress at break (120°C)
100
MPa
Stress at break (150°C)
90
MPa
Stress at break (160°C)
85
MPa
Stress at break (180°C)
80
MPa
Stress at break (200°C)
70
MPa
Strain at break
3.6
%
Strain at break (-40°C)
3.4
%
Strain at break (120°C)
8
%
Strain at break (150°C)
8.5
%
Strain at break (160°C)
8.6
%
Strain at break (180°C)
9
%
Strain at break (200°C)
9.3
%
Flexural modulus
9200
MPa
Flexural modulus (120°C)
4500
MPa
Flexural modulus (160°C)
4100
MPa
Flexural strength
290
MPa
Flexural strength (120°C)
135
MPa
Flexural strength (160°C)
115
MPa
Charpy impact strength (+23°C)
90
kJ/m²
Charpy impact strength (-30°C)
65
kJ/m²
Charpy notched impact strength (+23°C)
12
kJ/m²
Charpy notched impact strength (-30°C)
10
kJ/m²
Izod notched impact strength (+23°C)
10
kJ/m²
Puncture - maximum force (+23°C)
900
N
Puncture - maximum force (-30°C)
800
N
Puncture energy (+23°C)
2.8
J
Puncture energy (-30°C)
2.3
J
Weldline strength at thickness 1
100
MPa
Weldline strain at thickness 1
1.4
%
Thickness tested (1)
4
mm

Thermal properties

Melting temperature (10°C/min)
260
°C
Temp. of deflection under load (1.80 MPa)
250
°C
Temp. of deflection under load (0.45 MPa)
260
°C
Coeff. of linear therm. expansion (parallel)
0.2
E-4/°C
Coeff. of linear therm. expansion (normal)
0.7
E-4/°C
Relative Temperature Index - electrical
65
°C
RTI electrical (Thickness (1) tested)
0.71
mm
Relative Temperature Index - electrical
65
°C
RTI electrical (Thickness (2) tested)
3
mm
Relative Temperature Index - with impact
65
°C
RTI with impact (Thickness (1) tested)
0.71
mm
Relative Temperature Index - with impact
65
°C
RTI with impact (Thickness (2) tested)
3
mm
Relative Temperature Index - without impact
65
°C
RTI without impact (Thickness (1) tested)
0.71
mm
Relative Temperature Index - without impact
65
°C
RTI without impact (Thickness (2) tested)
3
mm

Electrical properties

Relative permittivity (100Hz)
3.8
-
Relative permittivity (1 MHz)
3.5
-
Dissipation factor (100 Hz)
90
E-4
Dissipation factor (1 MHz)
160
E-4
Volume resistivity
1E13
Ohm*m
Surface resistivity
Ohm
Electric strength
30
kV/mm
Comparative tracking index
600
V

Other properties

Water absorption
5.5
%
Humidity absorption
1.6
%
Density
1360
kg/m³

Rheological calculation properties

Thermal conductivity of melt
0.172
W/(m K)
Spec. heat capacity melt
2170
J/(kg K)

Diagrams

Applications

Spatulas and Kitchenware

Industry
Consumer goods
Stanyl® PA46 and Akulon® PA66 are reliable solutions for spatulas and other kitchenware. Stanyl PA46 offers much higher melting temperature and HDT than PA66, and both materials have significantly higher melting temperature resistance than PP and PA6. Also, Stanyl TE200F6-FC and EcoPaXX® Q-KG6-FC are food-approved.}